E44-1006 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Non-resistant choice, corrosion, leak
[Mechanism] Material was chosen by strength only, ignoring fluid corrosivity; carbon steel uniformly thinned over years in acid/salt spray and leaked.
[Calculation] Fluid pH=3, carbon-steel corrosion rate 2mm/a, 3 years thins 6mm, δ=8mm drops to 2mm, far below the 7mm needed.
[Design Omission] No corrosion-resistant material, no corrosion check, and no lining.
1) Re-select corrosion-resistant 316L (corrosion rate <0.05mm/a at pH=3), since carbon steel corrodes fast and a better steel eases it — thus preventing corrosion;
2) Check fluid corrosion resistance (select per GB/T fluid corrosion chart), since a non-resistant choice corrodes and the check protects it — thus material compliance;
3) Switch to stainless/duplex (2205 for carbon steel), since carbon corrodes and a better steel raises resistance — thus resisting corrosion;
4) Add a lining/coating (3mm rubber or PTFE), since a bare wall corrodes and a lining isolates it — thus isolating corrosion;
5) Run corrosion coupons (1a, weigh loss to set rate), since without measurement the rate is unknown and a coupon reveals it — thus grading the rate by data;
6) Perform periodic thickness measurement (every six months, repair if over 0.5mm loss), since thinning first shows as wall loss and can be replaced early — thus monitoring corrosion;
7) Hold fluid pH≥6 (suppress corrosion), since acidity promotes corrosion and fluid control eases it — thus running to prevent thinning;
8) Write the material selection and corrosion check into the spec, since the non-resistant-choice root cause was the missed fluid corrosion check — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels