E44-274 · Valve Selection and Internal Leakage · High-pressure globe valve J61Y-320 DN20 · ★★★
The seat Stellite hardfacing spalled over 4mm²; internal leakage was 0.5L/min, and high-pressure gas blew through.
[Spalling] Differential thermal expansion between the hardfacing and the base drove the interface stress above the bond strength, and the layer peeled.
[Erosion] The high-pressure, high-velocity flow scoured the spall pit and enlarged the leak.
[Design Omission] No control of the hardfacing process and preheat, and no bond inspection — the high-pressure valve leaked.
1) Preheat before hardfacing and cool slowly to control thermal stress; expansion mismatch drove the interface stress above bond strength and peeled 4mm², so bond it firmly;
2) Do dye penetrant testing on the hardfacing layer to find cracks; cracks are the start of spalling, so inspect for them;
3) Raise bond strength (a buffer layer) to prevent spalling; direct buildup peels easily, so add a transition layer;
4) For high-pressure high-velocity flow switch to a lapped metal seat and polish it; erosion enlarges the leak, so make it erosion-resistant;
5) Periodically measure internal leakage to detect spalling; spalling is gradual, so diagnose early;
6) Use a replaceable seat design for easy repair; once spalled the seat must be replaced, so make it renewable;
7) Control the medium velocity to cut erosion; high v erodes hard, so slow it down;
8) Bring the hardfacing process under quality control; the missing inspection was the cause of spalling, so gate the process.
GB/T 12224-2015 Steel valves — General requirements