E44-275 · Valve Selection and Internal Leakage · Rubber-lined diaphragm valve G41J-10 DN65 · ★★
The rubber lining blistered and debonded; the medium seeped to the substrate, the body cavity rusted, and internal leakage reached 0.8L/min.
[Debonding] Poor vulcanization left the rubber-to-steel bond strength < the medium osmotic pressure, causing blistering.
[Permeation] Pinholes in the lining let the medium seep along the seams to the substrate and rust it.
[Design Omission] No control of vulcanization or pinhole inspection, and no medium-compatible rubber chosen — the rubber-lined valve leaked.
1) Control vulcanization temperature and time so the bond strength meets spec; under-cure left the rubber-steel bond < osmotic pressure and blistered it, so bond it firmly;
2) Use spark testing at the factory to detect pinholes; holes let the medium seep to the substrate and rust it with 0.8L/min leakage, so check for holes;
3) Pick a corrosion-resistant rubber grade for the medium; a wrong match makes the rubber swell and detach, so make it chemical-resistant;
4) Sand-blast the substrate to a rough finish before lining; a smooth face bonds weakly, so raise the adhesion;
5) Periodically check for blisters and replace early; debonding is gradual, so diagnose early;
6) Add a drain port in the body cavity to prevent pooled liquid and rust; pooling accelerates substrate rust, so make it drainable;
7) Switch to a one-piece lining to cut seams; seams are the start of permeation, so reduce them;
8) Bring vulcanization and leak testing under quality control; the lack of control was the cause of debonding, so gate the process.
GB/T 12239-2008 Industrial valves - Metal diaphragm valves