E45-329 · Environmental Protection and Temperature/Humidity · Level Sensor · ★★
On a seaside platform, a carbon-steel housing rusts through in 3 months; salt spray enters through the rust holes and corrodes the circuit until it fails
[Mechanism] Chloride ions in the salt spray break down the passive film on the carbon steel and cause pitting; the loose rust layer flakes off and forms holes, through which salt spray and moisture enter and corrode the circuit.
[Calculation] The salt-spray corrosion rate of carbon steel in a marine atmosphere is about 0.1mm/month; over 3 months 0.3mm exceeds the corrosion allowance of a 1mm thin wall, so pitting perforates it.
[Design Omission] Carbon steel was selected without choosing a corrosion-resistance grade for the marine environment.
① Material matching: for marine salt spray → choose 316L stainless steel or add an epoxy coating → resist chloride pitting
② Surface protection: apply Dacromet or powder coating to the housing → isolate it from salt spray
③ Upgraded sealing: use fluoroelastomer O-rings at the seams → prevent salt-spray ingress
④ Sacrificial anode: add zinc blocks for cathodic protection → sacrifice them first to protect the body
⑤ Circuit protection: coat the board with conformal coating → no corrosion even with minor seepage
⑥ Corrosion monitoring: measure the wall thickness periodically and warn at <0.8mm → replace before perforation
⑦ Salt-spray verification: run a neutral salt-spray test for ≥720h with no rust-through → data confirmation
⑧ Selection standardization: write the environmental corrosion class into the material selection table → control at the source
GB/T 10125-2021 Corrosion tests in artificial atmospheres - Salt spray tests