E45-333 · Environmental Protection and Temperature/Humidity · Gas Sensor · ★★
In a chemical plant H2S gas sulfidizes and blackens the sensor's wiring terminals and internal contacts; contact resistance rises and the signal is attenuated
[Mechanism] H2S reacts with the copper and silver contacts to form a sulfide film; the film is highly resistive and raises contact resistance, so weak signals are divided down by the high resistance and attenuated.
[Calculation] At an H2S concentration of 10ppm the silver contacts sulfidize at about μm per month; after several months the film raises contact resistance from mΩ to the Ω level, and the voltage drop in the 24V loop becomes significant.
[Design Omission] The contact material was not selected for gold plating or sealing in a corrosive-gas environment.
① Gold-plated contacts: gold-plate the terminals and contacts → resist sulfidation and form no high-resistance film
② Sealed gas barrier: fill the wiring cavity with nitrogen or pot it → isolate the corrosive gas
③ Material upgrade: choose corrosion-resistant stainless steel with a coating for the housing → withstand H2S
④ Positive-pressure protection: maintain a slight positive pressure of clean air in the cabinet → keep the gas out
⑤ Contact monitoring: measure contact resistance and alarm at >50mΩ → early corrosion warning
⑥ Regular maintenance: clean the contacts and measure resistance periodically → prevent film buildup
⑦ Corrosion verification: run a mixed-gas corrosion test to confirm → data confirmation
⑧ Selection standardization: write gold-plated contacts for corrosive-gas environments into the selection spec → control at the source
GB/T 2423.51-2020 Environmental testing for electric and electronic products - Flowing mixed gas corrosion test