E45-345 · Environmental Protection and Temperature/Humidity · Underwater Level Sensor · ★★★
A dock underwater sensor immersed in seawater for a long time: crevice electrochemical corrosion of the stainless-steel housing perforates it, letting water in and shorting it
[Mechanism] Chloride ions in seawater cause crevice corrosion at the gaps in the stainless steel; once the passive film breaks down, the local potential difference accelerates pitting until perforation.
[Calculation] Seawater chloride is about 19g/L; 316L corrodes at roughly 0.05mm/month in the crevice, so in half a year 0.3mm penetrates the thin-wall seal.
[Design Omission] The material's corrosion-resistance grade was insufficient, with no crevice-corrosion protection.
① Material upgrade: for seawater immersion → choose titanium alloy or duplex steel → resist chloride crevice corrosion
② Seamless construction: weld into one piece to eliminate gaps → no crevice-corrosion sites
③ Cathodic protection: add sacrificial anode blocks → electrochemically protect the body
④ Coating isolation: apply a seawater-resistant coating to the housing → isolate contact
⑤ Upgraded sealing: multiple O-rings plus potting → prevent seepage
⑥ Corrosion monitoring: periodically measure wall thickness, warn when <0.8mm → replace before perforation
⑦ Immersion verification: run a seawater immersion test for ≥6 months without perforation → data confirmation
⑧ Selection standardization: write seawater-environment materials into the selection table → control at the source
GB/T 10125-2021 Corrosion tests in artificial atmospheres - Salt spray tests