E46-016 · Welding Process & Distortion · Dissimilar-Steel Joint · ★★★
Carbon steel was welded directly to stainless steel; a brittle hard layer formed in the fusion zone, cracked and leaked
[Mechanism] Direct welding of dissimilar steels drives carbon migration and forms a brittle hard layer that cracks under stress.
[Calculation] A fusion-zone hardness above HV350 causes embrittlement, cracking and leakage.
[Design gap] No transition layer or matching filler metal was used.
① Use a nickel-based transition layer: use a nickel-based filler as a transition layer when welding dissimilar steels to moderate the brittleness
② Select the filler by dissimilar combination: select the filler metal according to the dissimilar-steel combination to ensure matching
③ Control the heat input: reduce the heat input to cut carbon migration and lower embrittlement
④ NDT for cracks: inspect for cracks by NDT and correct them early
⑤ Joint mechanical test: carry out joint mechanical-property tests for early detection
⑥ Welding procedure qualification: re-qualify to confirm the procedure is feasible and the properties are ensured
⑦ Transition verification: confirm the transition-layer hardness meets the requirement by hardness measurement
⑧ Standardize process: write the transition-layer requirement into the welding procedure specification (WPS), controlling at the source
GB/T 19866-2005 General principles for welding procedure specification and qualification