E46-062 · Heat Treatment & Stress · Stainless-Steel Pressure Vessel · ★★★
A stainless-steel pressure vessel had its circumferential weld machined at the groove face without heat treatment after welding; after machining the shell ovality was 3mm, beyond the ≤1mm tolerance.
[Mechanism] The residual stress of the circumferential weld couples with the cutting force of machining, making the shell plastically deform into an oval.
[Calculation] The hoop residual stress of about 150MPa is released and the ovality exceeds 2mm.
[Design gap] No overall stress relief was carried out after welding as required by the specification.
① Overall stress relief after welding: after completing the circumferential weld carry out overall stress-relief heat treatment to release the stress evenly
② Local annealing: for parts that cannot be treated as a whole, do local annealing with a soak and slow cooling
③ Age before machining: complete the stress relief and let the part stabilize before machining
④ Increase the allowance: leave a larger allowance for machining and take several passes to reduce the cutting force
⑤ Support and restraint: restrain the shell with process supports during machining to limit distortion
⑥ Ovality check: measure the ovality during machining and repeat the stress relief if out of tolerance
⑦ Distortion verification: confirm it is within tolerance by ovality measurement
⑧ Standardize process: write post-weld stress relief into the process specification, controlling at the source
GB/T 150.4-2011 Pressure vessels - Part 4: Fabrication, inspection and acceptance