E46-061 · Heat Treatment & Stress · Welded Gearbox · ★★★
A welded gearbox housing was finish-machined directly after welding without stress relief; after 2 weeks the face had distorted 0.5mm and the assembly hole positions were off by 0.3mm, beyond tolerance.
[Mechanism] The welding residual stress is released once machining removes the constraint, causing the housing to distort as a whole.
[Calculation] The welding residual stress is about 200MPa, and its release distorts the part by more than 0.3mm.
[Design gap] No stress-relief annealing was arranged before machining.
① Stress-relief annealing after welding: after welding carry out stress-relief annealing (e.g. 550~600℃) to remove the welding stress
② Separate rough and finish machining: after rough machining relieve the stress again before finish machining to reduce the distortion from stress release
③ Control heating and soaking: heat and soak to specification and cool slowly to ensure the stress relaxes fully
④ Natural aging: for non-critical parts use outdoor open-air natural aging instead of heat treatment
⑤ Vibratory stress relief: use vibratory stress-relief equipment to remove the residual stress and shorten the cycle
⑥ Distortion monitoring: monitor the distortion before machining and re-anneal if out of tolerance
⑦ Distortion verification: after finish machining measure the distortion on a CMM to confirm it is within tolerance
⑧ Standardize process: write the post-weld stress-relief step into the process route, controlling at the source
GB/T 37405-2019 Welded components - Selection of process parameters and technical requirements for vibratory stress relief