E46-060 · Heat Treatment & Stress · 40Cr Spindle · ★★
A 40Cr spindle after quench-and-temper (quenching + tempering at 560℃) had a hardness of HRC24 (should be HRC28-32); the tensile strength of only 750MPa was below the required 900MPa, and it broke in bending under load.
[Mechanism] A tempering temperature that is too high or incomplete quenching leaves a coarse sorbite structure and insufficient strength.
[Calculation] A tempering temperature of 560℃ is on the high side and leaves the strength about 17% below the requirement.
[Design gap] Neither the quench-and-temper tempering temperature nor the quenching cooling rate was specified.
① Lower the tempering temperature: lower the quench-and-temper tempering temperature to the process lower limit (520~540℃ for 40Cr) to keep the strength
② Quench fully: use oil quenching with ensured cooling to obtain full martensite before tempering
③ Hardness spot check: spot-check the hardness after quench-and-temper to confirm HRC28-32
④ Tensile test: carry out a tensile test on the first piece to confirm a tensile strength ≥900MPa
⑤ Metallographic check: examine the fineness of the tempered sorbite to confirm acceptance
⑥ Re-quench and temper: re-do quench and temper on parts with insufficient strength
⑦ Performance verification: confirm the strength meets the requirement by hardness and tensile testing
⑧ Standardize process: write the quench-and-temper temperature into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel