E46-059 · Heat Treatment & Stress · 38CrMoAl Screw · ★★
A 38CrMoAl screw was plasma-nitrided for 60h and the white layer reached 12μm (should be ≤8μm); the surface peeled and spalled, and it seized after assembly.
[Mechanism] Too long a nitriding time or an improper ammonia dissociation rate forms an overly thick brittle compound white layer on the surface.
[Calculation] The 12μm white layer exceeds the 8μm limit and peels brittlely.
[Design gap] No upper limit was set on the white-layer thickness or the dissociation rate.
① Control the nitriding time: keep the plasma-nitriding time within the process range so the white layer is ≤8μm
② Adjust the dissociation rate: keep the ammonia dissociation rate at 15%~30% to reduce the brittle compound
③ White-layer check: after nitriding measure the white-layer thickness by metallography and regrind if out of tolerance
④ Denitriding treatment: reduce the ammonia flow in the later stage of nitriding for denitriding to thin the white layer
⑤ Precision grinding removal: precision-grind the surface brittle layer off parts with an overly thick white layer
⑥ Bonding check: do a Vickers indentation to check the bonding of the nitrided layer
⑦ Performance verification: confirm there is no peeling by white-layer thickness and bonding
⑧ Standardize process: write the nitriding time and dissociation rate into the process card, controlling at the source
GB/T 11354-2005 Iron and steel parts - Determination of nitrided case depth and metallographic examination