E46-058 · Heat Treatment & Stress · 20CrMnTi Gear · ★★
A 20CrMnTi gear was carburized for 18h to a case depth of 1.8mm (should be 0.8~1.2mm); the tooth root fractured brittlely along the carburized layer with a rock-candy intergranular fracture.
[Mechanism] Carburizing for too long makes the case too deep and the surface carbon content too high, leaving much retained austenite and great brittleness after quenching.
[Calculation] A case depth of 1.8mm exceeds the upper limit by 50%, and the brittleness rises markedly.
[Design gap] No upper limit was set on the carburizing soak.
① Set a carburizing upper limit: keep the carburizing soak within the process upper limit so the case depth does not exceed 1.2mm
② Lower the carbon potential: keep the furnace-atmosphere carbon potential at 0.8%~1.0% to avoid surface supersaturation
③ Case-depth spot check: check the case depth after carburizing and downgrade or rework out-of-tolerance parts
④ Double quenching: use double quenching on over-carburized parts to refine the structure and reduce retained austenite
⑤ Slow cooling: cool slowly after carburizing and then reheat to reduce stress
⑥ Metallographic check: examine the carbide network to confirm there is no anomaly
⑦ Performance verification: confirm there is no tendency to brittle fracture by case depth and impact toughness
⑧ Standardize process: write the carburizing upper limit into the process card, controlling at the source
GB/T 9450-2005 Determination and verification of the effective depth of hardening of carburized and hardened steel parts