E46-057 · Heat Treatment & Stress · 20CrMnTi Gear · ★★
A 20CrMnTi gear had a carburized case depth of 0.4mm (should be 0.8~1.2mm); after 3 months of running the tooth flanks spalled and the wear of 0.3mm was out of tolerance.
[Mechanism] Insufficient carburizing soak leaves the diffusion layer shallow, so the surface pressure capacity and wear resistance are inadequate.
[Calculation] A case depth of 0.4mm is 50% shallower than required, and the contact-fatigue life drops several-fold.
[Design gap] Neither the carburized case depth nor the carburizing rate was specified.
① Adequate carburizing time: calculate from the target case depth and lengthen the carburizing soak so the case depth reaches 0.8~1.2mm
② Control the carburizing temperature: hold the carburizing temperature at 920~930℃ to ensure the carbon potential
③ Case-depth check: spot-check the case depth after carburizing to confirm it is up to standard
④ Carbon-potential control: control the furnace-atmosphere carbon potential at 0.8%~1.0% with an oxygen probe
⑤ Matching quench: quench directly after carburizing or reheat and quench to obtain a hard surface layer
⑥ Metallographic check: examine the case and core structures to confirm acceptance
⑦ Performance verification: confirm the wear resistance by case depth and surface hardness
⑧ Standardize process: write the carburized case depth into the process card, controlling at the source
GB/T 9450-2005 Determination and verification of the effective depth of hardening of carburized and hardened steel parts