E46-056 · Heat Treatment & Stress · Q235 Structural Part · ★★
A Q235 structural part was normalized at 880℃ (should be 920℃); a grade-4 banded ferrite structure formed, the mechanical properties were uneven, and the heat-affected zone softened during welding.
[Mechanism] A normalizing temperature that is too low prevents the structure from fully austenitizing, and coarse, uneven banded ferrite forms on cooling.
[Calculation] Below Ac3 the transformation is incomplete and the banding exceeds grade 3.
[Design gap] Neither the normalizing temperature nor the cooling method was specified.
① Normalize to temperature: raise the normalizing temperature to 30~50℃ above Ac3 (about 920℃ for Q235) for full austenitizing
② Control air cooling: control the air-cooling rate after normalizing to ensure a uniform structure
③ Metallographic inspection: inspect the banded structure of every batch metallographically and require it to be finer than grade 3
④ Uniform heating: ensure uniform temperature in the furnace to avoid cold spots
⑤ Re-normalize: re-normalize parts with an unacceptable structure as a remedy
⑥ Mechanical re-inspection: re-inspect the mechanical properties to confirm uniformity
⑦ Structure verification: confirm the banded structure is acceptable by metallography
⑧ Standardize process: write the normalizing temperature into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel