E46-055 · Heat Treatment & Stress · Cast Bed · ★★★
A cast bed was only stress-relief annealed at 550℃ (should be 600℃/4h); one week after rough machining the face had distorted 0.6mm, exceeding the 0.1mm tolerance.
[Mechanism] Insufficient annealing temperature and time leave the residual stress incompletely relaxed, and it is released later during machining, causing distortion.
[Calculation] Annealing at 550℃ lowers the residual stress by only 40%, far from enough.
[Design gap] No lower limits were set on the annealing temperature and soak time.
① Adequate stress-relief annealing: anneal at 550~600℃ with a sufficient soak according to the casting wall thickness to relax the stress fully
② Control heating and soaking: heat at about 30℃ per hour and soak ≥4h to ensure the part is heated through
③ Slow cooling and unloading: cool in the furnace to below 200℃ before unloading to avoid new stress
④ Separate rough and finish machining: after rough machining relieve the stress again before finish machining to reduce distortion
⑤ Distortion monitoring: after rough machining let the part rest and monitor the distortion, re-annealing if out of tolerance
⑥ Stress measurement: spot-check the residual stress by the blind-hole method to confirm it has dropped
⑦ Distortion verification: after finish machining measure the distortion on a CMM to confirm it is within tolerance
⑧ Standardize process: write the annealing specification into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel