E46-054 · Heat Treatment & Stress · 40Cr Connecting Rod · ★★
A 40Cr connecting rod was quench-and-tempered with 6h tempering (should be 2h) at 600℃; the hardness dropped to HRC22, below the required HRC28-32, and it yielded and distorted after assembly.
[Mechanism] Too long a tempering time and too high a temperature let the carbides agglomerate and grow, softening the matrix.
[Calculation] Tempering for 6h instead of 2h lowers the hardness by about 8HRC, below the lower limit.
[Design gap] No upper limit was set on the tempering soak.
① Limit the tempering time: keep the tempering soak within the specified upper limit (2h for 40Cr) to prevent over-softening
② Control the tempering temperature: temper strictly at the drawing temperature and avoid overshoot
③ Hardness spot check: spot-check the hardness of every batch after tempering to confirm HRC28-32
④ Metallographic check: examine the tempered sorbite structure to confirm it has not over-aged and agglomerated
⑤ Process trial: carry out a mechanical-property test on the first piece to confirm the strength
⑥ Furnace temperature record: record the furnace temperature curve throughout for traceability
⑦ Performance verification: confirm the strength is acceptable by hardness and tensile testing
⑧ Standardize process: write the tempering time and temperature into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel