E46-053 · Heat Treatment & Stress · T10 Tool Steel Cutting Tool · ★★
A T10 cutting tool was tempered at only 150℃ after quenching (should be 220℃); the hardness HRC66 was above the required HRC58-62, and with an impact energy of only 8J the edge chipped in use.
[Mechanism] A tempering temperature that is too low leaves the martensite incompletely decomposed, with high residual stress and great brittleness.
[Calculation] Tempering at 150℃ leaves the martensite carbon content still high, and the impact energy is less than one third of normal.
[Design gap] Neither a minimum tempering temperature nor a soak time was specified.
① Temper at a higher temperature: raise the tempering temperature above the process lower limit (220℃ for T10) to lower the hardness adequately
② Lengthen the soak: ensure a tempering soak of ≥2h according to the workpiece thickness so the transformation completes
③ Hardness check: spot-check the hardness after tempering to confirm it is within HRC58-62
④ Impact test: carry out an impact test on the tool to confirm the toughness is adequate for service
⑤ Double tempering: use double tempering for high-alloy steels to remove the residual stress further
⑥ Controlled heating: heat the tempering furnace in stages to avoid thermal shock
⑦ Performance verification: confirm the tempering is adequate by hardness and impact energy
⑧ Standardize process: write the tempering temperature lower limit into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel