E46-052 · Heat Treatment & Stress · Thin-Walled Bearing Housing · ★★
A bearing housing with a 4mm wall thickness cracked into 3 pieces after water quenching, warped 2.5mm, and its roundness was out of tolerance by 0.8mm so it could not be machined.
[Mechanism] Too severe water-quench cooling generates huge thermal stress superimposed on the transformation stress, exceeding the material strength and causing cracking and warping.
[Calculation] The water-quench cooling rate is about 400℃/s, and the thermal stress exceeds 600MPa, above the yield strength.
[Design gap] The cooling medium of the thin-walled part was not selected by wall thickness.
① Switch to oil quenching: use quenching oil for thin-walled parts to cut the cooling rate to about 80℃/s and reduce the stress
② Interrupted quenching: use nitrate-salt interrupted quenching, holding near Ms to reduce the temperature difference
③ Control the water temperature: if water quenching is required, keep the water at 30~60℃ with agitation to avoid local over-cooling
④ Pre-distortion compensation: pre-set a counter-distortion on distortion-prone parts to offset the quenching distortion
⑤ Fixture restraint: hold the workpiece with a quenching fixture to limit warping
⑥ Timely tempering: temper promptly after quenching to remove the residual stress
⑦ Distortion verification: measure the distortion on a CMM after quenching to confirm it is within tolerance
⑧ Standardize process: write the cooling medium and method into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel