Too High a Quenching Temperature Causes Overheating Cracks

E46-051 · Heat Treatment & Stress · 45 Steel Gear · ★★

Problem Description

A 45 steel gear blank was quenched at 920℃ (normally 830℃); a network of cracks appeared on the tooth flank, the grain size was grade 1, and it cracked before assembly.

Root Cause

[Mechanism] A quenching temperature far above Ac3 makes the austenite grains grow drastically, and coarse martensite and network cracks form on cooling.
[Calculation] Overheating coarsens the grain size from grade 8 to grade 1, and the impact energy drops by more than 60%.
[Design gap] Neither an upper limit on the quenching temperature nor furnace temperature uniformity was specified.

Corrective Solution

① Strictly control the quenching temperature: limit the quenching temperature to Ac3 + 30~50℃ (about 830℃ for 45 steel) to avoid overheating
② Furnace calibration: calibrate the furnace temperature uniformity periodically so the actual workpiece temperature matches the instrument
③ Grain-size check: spot-check the grain size of every batch and require it to be finer than grade 5 to prevent a coarse structure
④ Normalize as a remedy: for overheated parts, normalize first to refine the grains, then re-quench to restore the properties
⑤ Control the heating time: control the soak by the effective thickness to limit grain growth
⑥ Metallographic monitoring: check metallographically at regular intervals and rework promptly if a network carbide is found
⑦ Performance verification: confirm the structure is acceptable by grain size and hardness testing
⑧ Standardize process: write the quenching temperature upper limit into the heat-treatment process card, controlling at the source

Checklist

Reference

GB/T 16923-2008 Normalizing and annealing of steel, and GB/T 6394-2017 Determination of average grain size of metals