E46-068 · Heat Treatment & Stress · 45 Steel Gear · ★★
A 45 steel gear was medium-frequency hardened to a case depth of 4.5mm (should be 2.5~3.5mm); sub-case spalling appeared on the tooth flanks and teeth broke off.
[Mechanism] Heating too deep concentrates stress in the transition zone between the hardened layer and the core, and the layer cracks brittlely and spalls.
[Calculation] The 4.5mm case depth exceeds the upper limit, and the shear stress in the transition zone exceeds the material strength.
[Design gap] No upper limit was set on the heating depth for surface hardening.
① Set a case-depth upper limit: control the medium-frequency parameters so the hardened layer does not exceed 3.5mm
② Optimize cooling: use a suitable quenching liquid to avoid soft spots below the case
③ Case-depth check: check the case depth after quenching and downgrade or regrind out-of-tolerance parts
④ Stress relief: temper promptly after quenching to reduce the interlayer stress
⑤ Rework: remachine spalled parts and re-quench them
⑥ Metallographic check: examine the transition-zone structure to confirm it is sound
⑦ Performance verification: confirm there is no spalling by case depth and bonding
⑧ Standardize process: write the case-depth upper limit into the process card, controlling at the source
GB/T 5617-2005 Determination of effective depth of hardening after induction or flame hardening of steel