E46-067 · Heat Treatment & Stress · 45 Steel Spindle · ★★
A 45 steel spindle was medium-frequency hardened to a case depth of 1.0mm (should be 2.5~3.5mm); after half a year of service the journal had worn 0.4mm, beyond tolerance, and the support failed.
[Mechanism] Insufficient induction-heating power or time leaves the hardened layer shallow, so the wear and load-carrying capacity is inadequate.
[Calculation] A 1.0mm case depth is 60% shallower than required, and the wear life drops sharply.
[Design gap] Neither the surface-hardening case depth nor the power parameters were specified.
① Adequate heating parameters: raise the medium-frequency power or lengthen the heating time so the hardened layer reaches 2.5~3.5mm
② Control the quenching liquid: ensure the quenching-liquid pressure and flow to obtain a sufficient cooling rate
③ Case-depth check: spot-check the hardened layer depth after quenching to confirm it is up to standard
④ Hardness gradient: check the hardness gradient to confirm a gentle transition
⑤ Re-quench as a remedy: surface-harden parts with a shallow case again
⑥ Metallographic check: examine the hardened-layer structure to confirm acceptance
⑦ Performance verification: confirm the wear resistance by case depth and surface hardness
⑧ Standardize process: write the heating parameters into the process card, controlling at the source
GB/T 5617-2005 Determination of effective depth of hardening after induction or flame hardening of steel