E46-066 · Heat Treatment & Stress · 80mm-Diameter Shaft · ★★
An 80mm-diameter shaft was quenched with only 15min soaking (should be ≥40min); the core hardness HRC30 was below the surface's HRC55, and the strength after quench-and-temper was insufficient.
[Mechanism] Insufficient soaking time leaves the core below the quenching temperature, so it does not transform fully to martensite on cooling.
[Calculation] The unhardened core gives a 25HRC hardness difference and lowers the load-carrying capacity.
[Design gap] The soaking time was not calculated from the effective thickness.
① Adequate soaking time: calculate the soaking time from the effective thickness of the workpiece (e.g. 1.5~2min/mm) to ensure it is heated through
② Control the heating temperature: reach the quenching temperature and soak so the core austenitizes
③ Core check: spot-check the core hardness after quenching to confirm through-hardening
④ Sufficient cooling: use a suitable quenching medium to ensure the core cooling rate
⑤ Re-quench as a remedy: reheat and re-quench parts that did not harden through
⑥ Metallographic check: examine the core structure to confirm the martensite fraction
⑦ Performance verification: confirm through-hardening acceptance by the core hardness
⑧ Standardize process: write the soaking-time formula into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel