E46-065 · Heat Treatment & Stress · 2mm Thin-Plate Die · ★★
A 2mm thin-plate stamping die was preheated and heated at 300℃/h (should be ≤80℃/h); it cracked into 3 pieces as soon as it entered the furnace, with radial cracks from the corners.
[Mechanism] Heating too fast creates a large temperature difference between the inside and outside of a thin-walled part, and the thermal stress exceeds the cracking strength.
[Calculation] A 300℃/h heating rate raises the thermal stress above 400MPa, higher than the thin part's strength.
[Design gap] No upper limit was set on the heating rate for thin-walled parts.
① Limit the heating rate: keep the heating rate of thin-walled parts within 80℃/h to reduce the temperature difference
② Staged soaking: provide staged soaks at 300℃ and 600℃ for uniform heating
③ Furnace loading method: lay thin parts flat or hang them to avoid adding self-weight stress
④ Furnace temperature uniformity: ensure uniform temperature in the furnace to avoid local overheating
⑤ Charging temperature: keep the difference between the charging temperature and the workpiece small
⑥ Crack inspection: inspect for cracks during heating and stop if any are found
⑦ Heating verification: confirm the rate is compliant by the temperature curve
⑧ Standardize process: write the heating rate into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel