E46-073 · Heat Treatment & Stress · 40Cr Shaft Journal · ★★
The journal of a 40Cr shaft was high-frequency hardened at excessive power; the surface temperature exceeded 1000℃, circumferential cracks appeared after quenching, and 5 pieces were scrapped.
[Mechanism] Excessive high-frequency power overheats the surface layer; the structure coarsens and the thermal stress rises sharply, causing quenching cracks.
[Calculation] A surface above 1000℃ causes overheating and raises the cracking rate markedly.
[Design gap] No upper limit was set on the high-frequency power or the heating temperature.
① Limit the high-frequency power: keep the high-frequency hardening power within the process range so the surface temperature does not exceed Ac3 by much
② Control the heating temperature: monitor the surface temperature with an infrared pyrometer to avoid overheating
③ Optimize cooling: use a suitable quenching liquid and controlled spraying to reduce thermal shock
④ Timely tempering: temper at low temperature immediately after quenching to relieve stress
⑤ Crack inspection: after quenching inspect the circumferential cracks by magnetic-particle testing
⑥ Rework: remove the defects from cracked parts and re-quench
⑦ Quality verification: confirm there is no cracking by flaw detection
⑧ Standardize process: write the high-frequency power upper limit into the process card, controlling at the source
GB/T 5617-2005 Determination of effective depth of hardening after induction or flame hardening of steel