E46-076 · Heat Treatment & Stress · High-Speed Steel Cutting Tool · ★★
A high-speed steel cutting tool was quenched in a salt bath without adequate deoxidation; a 0.15mm decarburized layer formed on the surface, the edge hardness dropped, and the tool chipped during cutting.
[Mechanism] Oxides and sulfates in the salt bath decarburize the workpiece surface, leaving the cutting edge underhardened.
[Calculation] A 0.15mm decarburized layer lowers the cutting-edge hardness by about 10HRC, causing cutting failure.
[Design gap] The salt bath was neither deoxidized periodically nor chemically analyzed.
① Periodic deoxidation: add a deoxidizer (such as silicon-calcium-iron) to the salt bath at regular intervals and stir thoroughly
② Chemical analysis control: analyze the oxide content of the salt bath periodically and deoxidize as soon as it exceeds the limit
③ Settle and skim: after deoxidation let the bath settle and skim off the floating slag to purify it
④ Preheat and protect: preheat the workpiece and insert it into the salt bath quickly to reduce oxidation
⑤ Decarburization check: after quenching measure the decarburized layer by metallography and regrind if it is out of tolerance
⑥ Surface hardness: spot-check the cutting-edge hardness to confirm acceptance
⑦ Quality verification: confirm there is no decarburization by the decarburized layer and hardness
⑧ Standardize process: write the deoxidation regime into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel