E46-079 · Heat Treatment & Stress · 40Cr Spring · ★★★
40Cr springs were zinc-plated without hydrogen removal; after 1 week's storage 2 parts broke, with flat fracture surfaces characteristic of hydrogen embrittlement.
[Mechanism] Hydrogen is absorbed during plating; without hydrogen removal it collects at the grain boundaries and causes hydrogen-embrittlement delayed fracture under stress.
[Calculation] Parts without hydrogen removal show a significant hydrogen-induced delayed fracture rate after 1 week's storage.
[Design gap] No hydrogen-removal step was specified after plating for high-strength parts.
① Remove hydrogen after plating: promptly bake high-strength parts after plating (e.g. 200℃×2h)
② Control the plating bath: optimize the bath and current to reduce hydrogen absorption
③ Timing of hydrogen removal: remove hydrogen as soon as possible after plating, within 4h
④ Strength classification: for ultra-high-strength parts apply strict hydrogen removal and inspection
⑤ Delayed-fracture check: store and observe for delayed fracture
⑥ Hydrogen content: when necessary measure the hydrogen content to confirm it meets the requirement
⑦ Quality verification: confirm there is no hydrogen embrittlement by a delayed-fracture test
⑧ Standardize process: write the hydrogen-removal step into the process card, controlling at the source
GB/T 5267.1-2002 Fasteners - Electroplated coatings