E46-078 · Heat Treatment & Stress · 35CrMo Connecting Rod · ★★
A 35CrMo connecting rod was quench-and-tempered with insufficient tempering; the structure was tempered martensite instead of sorbite, the impact energy was only 25J versus the required 60J, and it fractured.
[Mechanism] The tempering temperature was too low or the time too short, so the martensite did not fully decompose into sorbite and the toughness is poor.
[Calculation] Insufficient tempering leaves the impact energy 42% below the requirement, making brittle fracture likely.
[Design gap] Neither a sorbite structure nor its inspection was specified for the tempered part.
① Adequate-temperature tempering: raise the tempering temperature and time until the structure converts to tempered sorbite
② Control the tempering temperature: follow the drawing's tempering temperature strictly and avoid running low
③ Metallographic check: after tempering confirm the sorbite structure by metallography and rule out retained martensite
④ Impact test: carry out an impact test to confirm the toughness meets the requirement
⑤ Re-quench and temper: re-do quench and temper on parts with an unacceptable structure
⑥ Furnace temperature record: record the furnace temperature curve for traceability
⑦ Quality verification: confirm the toughness by metallography and impact testing
⑧ Standardize process: write the tempering structure requirement into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel