Knowledge Base › Process and Assembly Error Case Study › No Normalizing After Carburizing Leaves Excess Retained Austenite

No Normalizing After Carburizing Leaves Excess Retained Austenite

E46-081 · Heat Treatment & Stress · 20CrMnTi Gear · ★★

Problem Description

A 20CrMnTi gear was quenched directly after carburizing without normalizing; the retained austenite of 35% was excessive, the surface hardness of HRC52 was below the required HRC58, and the wear resistance was poor.

Root Cause

[Mechanism] Without normalizing after carburizing the grains are coarse and the carbon concentration gradient is steep, so too much retained austenite remains after quenching.
[Calculation] A retained austenite content of 35% lowers the surface hardness by about 6HRC.
[Design gap] No normalizing to refine the structure before quenching was arranged after carburizing.

Corrective Solution

① Normalize after carburizing: normalize first to refine the grains and even out the carbon concentration, then quench
② Control the carbon potential: lower it in the late stage of carburizing to reduce surface supersaturation
③ Reheat: use reheat quenching rather than direct quenching to refine the structure
④ Retained austenite check: after quenching measure the retained austenite by metallography; if out of tolerance, rework
⑤ Cold treatment: apply additional cold treatment to parts with excess retained austenite
⑥ Surface hardness: spot-check the surface hardness to confirm it meets the requirement
⑦ Quality verification: confirm acceptability by retained austenite content and hardness
⑧ Standardize process: write normalizing after carburizing into the process card, controlling at the source

Checklist

Reference

GB/T 9450-2005 Determination and verification of the effective depth of hardening of carburized and hardened steel parts

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »