E46-082 · Heat Treatment & Stress · 38CrMoAl Screw · ★★
A 38CrMoAl screw was gas-nitrided at 480℃ (should be 510℃); the case depth was only 0.25mm, below the required 0.4mm, and the bearing surface wore prematurely.
[Mechanism] A low nitriding temperature slows nitrogen diffusion, giving a shallow case with insufficient surface hardness and wear resistance.
[Calculation] A 30℃ lower temperature reduces the diffusion rate by about 40% and the case depth falls short.
[Design gap] No lower limit was specified for the nitriding temperature.
① Raise the nitriding temperature: raise the gas nitriding temperature to the process lower limit (510℃ for 38CrMoAl)
② Control ammonia dissociation: control the ammonia dissociation rate to maintain an active nitrogen potential
③ Case depth check: after nitriding measure the case depth and confirm it is ≥0.4mm
④ Hardness spot check: spot-check the surface hardness to confirm it meets the requirement
⑤ Re-nitride: re-nitride parts with a shallow case as a remedy
⑥ Metallographic check: examine the case structure to confirm it is acceptable
⑦ Quality verification: confirm the wear resistance by case depth and hardness
⑧ Standardize process: write the nitriding temperature into the process card, controlling at the source
GB/T 11354-2005 Iron and steel parts - Determination of nitrided case depth and metallographic examination