E46-099 · Heat Treatment & Stress · 60Si2Mn Spring · ★★
The 60Si2Mn spring was quenched and tempered at 380℃ (should be medium-temperature 460℃); the hardness of HRC52 was too high and the elasticity insufficient, and it took a permanent set beyond tolerance after two months in service.
[Mechanism] Too low a tempering temperature leaves the structure largely martensitic, with insufficient elastic limit, and it creeps under long-term load.
[Calculation] Tempering at 380℃ lowers the elastic limit by about 15% compared with 460℃.
[Design gap] The medium-temperature tempering temperature was not specified.
① Medium-temperature tempering: raise the spring tempering temperature into the medium range (460℃ for 60Si2Mn) to obtain tempered troostite
② Control the tempering temperature: temper strictly at the temperature on the drawing to preserve the elastic limit
③ Hardness spot check: after tempering check the hardness and confirm it is in the HRC44-48 range
④ Elasticity test: carry out an elastic limit and permanent set test to confirm
⑤ Re-temper: re-temper nonconforming parts at medium temperature
⑥ Metallographic check: examine the tempered troostite structure to confirm
⑦ Quality verification: confirm acceptable elasticity by hardness and elasticity testing
⑧ Standardize process: write the medium-temperature tempering temperature into the process card, controlling at the source
GB/T 1222-2016 Spring steels