Knowledge Base › Process and Assembly Error Case Study › Incomplete Annealing of Cast Iron Leaves White Iron

Incomplete Annealing of Cast Iron Leaves White Iron

E46-098 · Heat Treatment & Stress · HT250 Casting · ★★

Problem Description

An HT250 casting was not fully annealed, white iron remained in the surface layer with a hardness of HB400, which made drilling difficult and chipped the cutting tool.

Root Cause

[Mechanism] Insufficient annealing leaves the cementite ungraphitized; the white iron structure is hard, brittle and difficult to machine.
[Calculation] A hardness of HB400 in the white iron zone far exceeds the machinable range.
[Design gap] No adequate graphitizing annealing was carried out.

Corrective Solution

① Full graphitizing annealing: graphitize the casting so the cementite decomposes into graphite
② Control the annealing temperature: heat up and hold to specification to ensure the cementite decomposes
③ Slow cooling: cool slowly after annealing to avoid reforming white iron
④ Hardness check: after annealing check the hardness to confirm machinability
⑤ Metallographic check: examine the graphite morphology to confirm there is no white iron
⑥ Re-anneal: re-graphitize castings that still contain white iron
⑦ Quality verification: confirm machinability by hardness and metallography
⑧ Standardize process: write the annealing specification into the process card, controlling at the source

Checklist

Reference

GB/T 9439-2010 Grey cast iron castings