E46-209 · Bonding & Sealing · Pipe flange · ★★
During servicing of a pipe flange, an old asbestos-rubber gasket with permanent compression marks was reused; even after retightening, water still seeped along the old marks, and tightening to the upper torque limit had no effect.
[Mechanism] The old gasket had already developed permanent plastic compression marks and hardened, losing its resilience; re-compressing it cannot fill the microscopic irregularities of the flange face.
[Calculation] The old gasket's resilience is less than 30% of a new one, and the contact pressure cannot reach what sealing requires.
[Design gap] Single-use of gaskets was not specified, and old parts were reused during servicing.
① Single use: replace the gasket with a new one once it is removed; never reuse it
② Select the material: choose a temperature- and pressure-resistant gasket material according to the medium, temperature, and pressure
③ Clean the faces: before assembly, clean old adhesive and debris off the flange faces to keep them flat
④ Center it: center the gasket without offsetting it, covering the sealing face
⑤ Tighten symmetrically: tighten the bolts in a diagonal cross sequence and in stages
⑥ Pressure test: after assembly, run a hydrostatic test to confirm no leakage
⑦ Sealing verification: confirm no leakage by pressure test
⑧ Standardize process: write single-use of gaskets into the servicing procedure
GB/T 9126 Non-metallic flat gaskets for pipe flanges