E46-213 · Bonding & Sealing · Nameplate bonding · ★
The equipment nameplate was bonded with a mix of double-sided tape and structural adhesive, applied only as dots at the four corners; after vibration in service the nameplate fell off, with the effective bonding area less than 20% of the total area.
[Mechanism] The bonding load capacity is proportional to the effective bonding area; dot bonding makes the actual load-bearing area too small, and the stress per unit area exceeds the limit, causing debonding.
[Calculation] The design calls for full bonding, but the actual dot-bonding area is about 15%, so the unit stress exceeds the adhesive's allowable value several times over.
[Design gap] Full bonding or a sufficient overlap area was not specified.
① Full bonding first: for nameplate-type bonding, use full adhesive coverage or a large enough overlap area
② Increase overlap: increase the sleeve or overlap length of load-bearing parts to raise the area
③ Double-sided tape as an aid: use structural double-sided tape for temporary positioning, then back it up with structural adhesive
④ Clean the surfaces: degrease and strip paint from the bonding surfaces to ensure a good bond
⑤ Pressurize during curing: use clamps or weights to ensure close contact
⑥ Strength check: perform a pull-off test to confirm no debonding
⑦ Bonding verification: confirm compliance by pull-off force
⑧ Standardize process: write the bonding-area requirement into the drawing
GB/T 7124-2008 Adhesives - Determination of tensile shear strength (rigid material to rigid material)