E46-216 · Bonding & Sealing · Ceramic tile bonding · ★★
The ceramic wear plate was glued in place; to level it, adhesive was applied too thickly in one pass (about 5mm), so after curing the adhesive layer contained many internal voids, sounded hollow when tapped, and the whole plate was prone to fall off.
[Mechanism] When the adhesive layer is too thick, internal solvent or reaction bubbles cannot float up and escape, and get trapped in the adhesive to form voids, weakening the bond.
[Calculation] The adhesive-layer thickness should be 1~2mm, but the measured value was 5mm; the porosity rose markedly and the effective area dropped.
[Design gap] The adhesive thickness was not controlled, and a thick adhesive layer was used to level the surface.
① Control adhesive thickness: keep the applied thickness at 1~2mm and do not use thick adhesive to level the surface
② Level the substrate: if the base is uneven, machine it flat first, then apply adhesive thinly
③ De-air and scrape flat: after applying, scrape flat to release all trapped air
④ Apply in passes: where the thickness difference is large, apply several thin passes and laminate them
⑤ Pressurize: use pressure-sensitive tape or weights to expel bubbles
⑥ Tap test: after curing, tap to check for hollow sound and debonding
⑦ Bonding verification: confirm soundness by tapping and pull-off
⑧ Standardize process: write the adhesive thickness into the process card
GB/T 7124-2008 Adhesives - Determination of tensile shear strength (rigid material to rigid material)