E46-217 · Bonding & Sealing · Laminated board · ★★
A multi-layer laminated board was bonded and cured in a press; because the backing plate was uneven and the pressure point was off-center, after curing the adhesive layer was thick on one side and thin on the other - the thin side debonded and the thick side ran short of adhesive.
[Mechanism] Uneven curing pressure unbalances the adhesive-layer thickness distribution: the thin spot runs short of adhesive and the thick spot has excess, so the bond is uneven.
[Calculation] Once the pressure deviation exceeds 20%, the adhesive-layer thickness difference exceeds a factor of two, and the thin side has poor contact.
[Design gap] The press parallelism and the backing-plate flatness were not calibrated.
① Calibrate the press: periodically calibrate the press platen parallelism and pressure uniformity
② Flat backing plate: use a flat backing plate to ensure uniform pressure
③ Even pressure control: apply pressure evenly according to the multi-point pressure readings
④ Limit blocks: add equal-height limit blocks to control the adhesive-layer thickness
⑤ Process monitoring: monitor pressure and temperature uniformity during curing
⑥ Section inspection: section random samples to check adhesive-layer uniformity
⑦ Bonding verification: confirm adhesive-layer uniformity by section inspection
⑧ Standardize process: write the uniform-pressure requirement into the process
GB/T 7124-2008 Adhesives - Determination of tensile shear strength (rigid material to rigid material)