E46-222 · Bonding and Sealing · Honeycomb Sandwich Panel · ★★
When bonding the face sheet of a honeycomb sandwich panel, the adhesive was applied and the parts were pressed together directly without roller or vacuum de-airing; large areas of bubbles remained in the adhesive layer, and the face sheet bulged locally and debonded under load.
[Mechanism] When the parts are pressed together the air in the adhesive layer is not fully expelled; the bubbles occupy bond area and form local voids that weaken the joint.
[Calculation] The bubbles cover about 25% of the bond face, reducing the effective load-bearing area accordingly.
[Design gap] No roller de-airing or vacuum compaction step was specified.
① Roller de-airing: after pressing together, roll from the center outward to expel the air
② Vacuum compaction: use a vacuum bag to compact the joint and remove trapped air
③ Even application: spread the adhesive evenly to avoid local starvation and air pockets
④ In-process check: look for bulges and bubbles during bonding
⑤ Tap test: tap after curing to check for hollow sounds
⑥ Section inspection: cut samples to check the porosity
⑦ Bond verification: confirm the porosity is acceptable by section inspection
⑧ Standardize process: write the de-airing step into the process
GB/T 7124-2008 Adhesives - Determination of tensile shear strength (rigid material to rigid material)