E46-237 · Bonding and Sealing · High-Pressure Cylinder · ★★★
A high-pressure cylinder used an O-ring; the working pressure reached 25MPa and the fitting clearance was too large, so the O-ring was extruded into the gap and cut into a jagged shape, and it leaked at high pressure.
[Mechanism] When the pressure is too high and the clearance is too large, the O-ring is forced into the gap and sheared, causing extrusion damage.
[Calculation] The clearance should be no more than 1/10 of the cord diameter; the measured clearance is more than twice that, so the extrusion risk is high.
[Design gap] No back-up ring was added for the high-pressure condition and the clearance was not controlled.
① Add a back-up ring: fit a PTFE back-up ring on the high-pressure side to prevent extrusion
② Control the clearance: keep the fitting clearance no more than 1/10 of the cord diameter
③ Choose the cord diameter: choose a ring with a cord diameter sufficient for the pressure
④ Check the squeeze: keep the compression rate within the design range
⑤ Pressure test: perform a high-pressure hold test
⑥ Strip and inspect: after the pressure test, dismantle and check that the ring has no extrusion damage
⑦ Sealing verification: confirm no leakage by pressure holding
⑧ Standardize process: write the back-up ring and clearance into the drawing
GB/T 3452.3-2005 Rubber O-rings - Groove dimensions