E46-244 · Bonding and Sealing · Glass Bonding · ★★
Glass was bonded to metal with a primer plus structural adhesive; the main adhesive was applied before the primer had dried to touch, the two layers dissolved into each other and stayed tacky without curing, the bond was weak and it came apart with a light pull.
[Mechanism] Applying the main adhesive over a wet primer lets the solvents dissolve into each other, so the interface does not separate into layers and curing is hindered, giving a weak bond.
[Calculation] Insufficient primer drying markedly lowers the interface strength, bringing the bond close to failure.
[Design gap] The main adhesive was applied without waiting for the primer to dry to touch.
① Wait for tack-dry: let the primer dry to touch as instructed before applying the main adhesive
② Control the environment: keep temperature and humidity favorable for primer drying
③ Thin primer: apply the primer thin and even, without puddling
④ Sample test: make a sample first to confirm curing
⑤ Strength check: perform a pull-off test
⑥ Interface check: check the interface for tackiness or intermixing
⑦ Bond verification: confirm acceptance by the pull-off result
⑧ Standardize process: write the tack-dry requirement into the process card
GB/T 7124-2008 Adhesives - Determination of tensile shear strength (rigid material to rigid material)