Knowledge Base › Process and Assembly Error Case Study › Excessive Grinding Feed Causing Burn

Excessive Grinding Feed Causing Burn

E46-264 · Machining Process · Surface Grinder · ★★

Problem Description

Surface grinding was fed at 0.05mm/pass (should be ≤0.02); the temperature rose in the wheel-workpiece contact arc, blue-purple burn bands appeared on the surface, and the surface hardness dropped.

Root Cause

[Mechanism] A large feed sharply increases grinding heat; the surface is tempered and burned, changing its structure.
[Calculation] Doubling the feed raises the removal rate, and the arc-zone temperature exceeds the tempering threshold.
[Design gap] Neither a grinding feed limit nor adequate cooling was specified.

Corrective Solution

① Limit the feed: take the finish-grinding feed to the small side of the process upper limit
② Split rough and finish: separate rough and finish grinding to reduce heat
③ Ample cooling: flush the arc zone with a high-flow coolant during grinding
④ Choose the wheel: select a wheel of suitable hardness for the material
⑤ Dress often: dress the wheel in time to keep it sharp
⑥ Check for burn: inspect for burn by flaw detection or acid pickling
⑦ Structure verification: confirm no burn by hardness or metallography
⑧ Standardize process: write the grinding feed into the process card, controlling at the source

Checklist

Reference

GB/T 2481.1-1998 Bonded abrasives - Grain sizes of abrasive