E46-265 · Machining Process · Cylindrical Grinder · ★★
Stainless steel was ground with a fine-grit wheel; the grinding chips readily loaded the wheel, the grinding force rose, the surface was torn, and frequent dressing was needed, hurting efficiency.
[Mechanism] A fine grit is too dense with little chip room, so tough, sticky chips clog the pores and the wheel loses its cutting ability.
[Calculation] For stainless steel a grit of 60 or finer gives insufficient chip room, and the loading rate rises markedly.
[Design gap] The wheel grit and structure were not selected according to the material.
① Choose the grit: for stainless steel choose a coarser grit to increase chip room
② Choose the structure: use an open-structure wheel for better chip clearance
③ Choose the abrasive: use a loading-resistant abrasive such as monocrystalline corundum
④ Ample cooling: use cutting fluid when grinding to reduce sticking
⑤ Dress often: dress as soon as loading occurs to restore sharpness
⑥ Trial grind: trial-grind and check chip clearance before deciding
⑦ Surface verification: confirm by a surface free of tearing
⑧ Standardize process: write the wheel specification into the process card, controlling at the source
GB/T 2481.1-1998 Bonded abrasives - Grain sizes of abrasive