E46-332 · Casting & Forging · Die Forging · ★★
The ribs and corners of a die forging were not fully filled; the underfill was 1.5mm deep and the contour was incomplete.
[Mechanism] Insufficient billet volume or press tonnage leaves the metal short of the far end of the die cavity.
[Calculation] If the billet volume is less than the cavity volume plus flash, underfill results; filling improves with tonnage and temperature.
[Design gap] The billet volume and equipment capability were not checked.
① Check billet volume: size the billet from the cavity volume plus flash
② Raise press tonnage: select equipment with enough tonnage to ensure filling
③ Control temperature: adequate temperature maintains flowability
④ Provide overflow: add overflow pockets at the corners to collect metal
⑤ Filling check: inspect the contour on die opening, detecting problems early
⑥ Adjust the process: add material or increase the blow force
⑦ Filling verification: confirm the absence of underfill by the contour
⑧ Standardize process: write the billet volume into the process card, controlling at the source
GB/T 12361-2016 Steel die forgings - Process