E46-359 · Surface Treatment & Coating · Aluminum part · ★★
The aluminum part's surface was scratched through to the substrate after anodizing; the film thickness was only 8μm (should be 15μm) because the sulfuric acid concentration and current were too low.
[Mechanism] Low anodizing current density and short time leave the film thin, so wear and corrosion resistance are poor.
[Calculation] Film thickness grows about 1.5μm/(A·dm²·min); a low current leaves the film thin.
[Design gap] Current and time were not calculated from the film-thickness requirement.
① Set current: calculate the current density of 1.5A/dm² from the target film thickness to reach full thickness
② Control time: set the anodizing time according to the film thickness to ensure thickness
③ Control concentration: keep the sulfuric acid concentration steady at 180g/L for uniform film formation
④ Film-thickness check: use eddy-current thickness measurement to check for ≥15μm and detect problems early
⑤ Re-anodize: re-anodize thin-film parts to restore wear resistance
⑥ Control sealing: hot-water seal after anodizing to improve corrosion resistance
⑦ Film-thickness verification: confirm meeting spec by thickness measurement, confirmed by data
⑧ Standardize process: write the process parameters into the anodizing specification, controlling at the source
GB/T 8013.1-2018 Anodic oxide coatings on aluminium and aluminium alloys