E46-358 · Surface Treatment & Coating · Steel Member · ★★
After hot-dip galvanizing, a steel member showed localized exposed iron and rusting; the average zinc coating thickness was 55μm (should be 85μm) because the galvanizing time was too short.
[Mechanism] A short galvanizing time and uneven fluxing produce a thin zinc layer with an inadequate barrier.
[Calculation] Every 30μm reduction in zinc thickness cuts the corrosion life by roughly one third; 55μm is on the thin side.
[Design gap] The galvanizing time and withdrawal speed were not controlled.
① Control galvanizing time: set it to 3-5 min according to wall thickness to keep the layer thickness
② Control withdrawal: withdraw uniformly at 1 m/min for an even zinc layer
③ Fluxing: apply the flux evenly to prevent exposed iron
④ Check coating thickness: use a magnetic thickness gauge to verify an average ≥85μm, detecting problems early
⑤ Re-galvanize: touch up or re-galvanize thin areas to restore the barrier
⑥ Control pretreatment: pickle off the rust cleanly before fluxing to preserve bonding
⑦ Thickness verification: confirm compliance with a thickness gauge, verified by data
⑧ Standardize process: write the galvanizing parameters into the galvanizing procedure, controlling at the source
GB/T 13912-2020 Metallic coatings - Hot dip galvanized coatings on fabricated iron and steel articles