E46-385 · Surface Treatment & Coating · Powder-coated part · ★★
The powder-coated part powdered and discolored from overcuring; the oven temperature of 240℃ exceeded the specified 200℃, degrading the resin.
[Mechanism] Overcuring degrades the resin, causing powdering, loss of gloss and discoloration.
[Calculation] Above 220℃ degradation increases every 10 minutes, causing powdering.
[Design gap] The oven temperature limit and line speed were not controlled.
① Control the limit: keep the oven temperature below 210℃ to prevent degradation
② Control line speed: keep the line speed high enough for adequate time without excess, for solid curing
③ Measure oven temperature: use an oven temperature tracker to measure in situ and prevent deviation
④ Powdering check: check the surface for absence of powder to detect problems early
⑤ Re-cure: re-cure overcured parts at a lower temperature to restore properties
⑥ Control pretreatment: keep phosphating sound to preserve adhesion
⑦ Appearance verification: confirm absence of powdering by visual inspection, confirmed by data
⑧ Standardize process: write the temperature limit into the powder process, controlling at the source
GB/T 21782.1-2008 Coating powders - Part 1