Powder Coating Under-Cured, Poor Adhesion

E46-399 · Surface Treatment & Coating · Powder-coated part · ★★

Problem Description

The powder-coated part lost coating on impact; the cure was insufficient, the coating did not cross-link, and adhesion was poor.

Root Cause

[Mechanism] Insufficient curing leaves the coating uncross-linked, brittle and poorly adherent.
[Calculation] With under-cure the cross-link density is low and the coating peels off on impact.
[Design gap] The cure profile and line speed were not controlled.

Corrective Solution

① Cure fully: use an adequate oven temperature profile to ensure cross-linking
② Control line speed: keep the line speed slow enough for stable curing
③ Measure oven temperature: measure the actual part temperature with a data tracker to prevent deviation
④ Adhesion check: impact-test to confirm no peeling, detecting problems early
⑤ Re-cure: re-cure under-cured parts and re-check their properties
⑥ Control pretreatment: keep phosphating sound to preserve adhesion
⑦ Performance verification: confirm meeting spec by impact testing, confirmed by data
⑧ Standardize process: write the curing profile into the powder procedure, controlling at the source

Checklist

Reference

GB/T 21782.1-2008 Coating powders - Part 1