E46-415 · Commissioning & Run-In · Spindle bearing · ★★★
The bearing was oil-bath heated to 160℃ and then assembled; after running, the inner-ring hardness dropped and the raceway spalled early.
[Mechanism] Heating above 120℃ tempers and softens the bearing steel, lowering hardness and load capacity.
[Calculation] Above 120℃ the hardness drops about 2 HRC for every 20℃ rise, shortening life.
[Design gap] The heating upper limit and temperature measurement were not controlled.
① Control the upper limit: keep the heating temperature below 100℃, preferably 80℃ to 100℃
② Measure temperature: monitor in real time with a thermocouple and take the bearing out as soon as it reaches temperature
③ Even heating: stir the oil while heating for uniform temperature and prevent local overheating
④ Assemble quickly: slip the bearing on immediately after removal to avoid jamming as it cools
⑤ Check hardness: spot-check the hardness after assembly and replace if it is below the original value
⑥ Control time: estimate the heating time from the bore diameter and do not overheat
⑦ Quality verification: confirm acceptance by the temperature record and hardness, confirmed by data
⑧ Standardize process: write the upper temperature limit into the assembly process, controlling at the source
GB/T 307.1-2017 Rolling bearings - Radial bearings - Tolerances