Tensile/compressive stress: σ = N/(lw·t) ≤ fwt
Shear stress: τ = V/(lw·t) ≤ fvv
Bending + shear: √(σ²+3τ²) ≤ 1.1·fwt
N — axial force (N)
V — shear force (N)
M — bending moment (N·mm)
lw — effective weld length (mm) (actual length minus 2× leg, and ≥10t)
t — thickness of thinner plate (mm)
fwt — design tensile strength of butt weld (MPa)
Base metal Q235 + E43 electrode: fwt=185MPa
Base metal Q345 + E50 electrode: fwt=265MPa
Base metal Q390 + E55 electrode: fwt=295MPa
When weld strength equals base metal strength (grade 1/2 weld), no calculation needed
Grade 3 weld (general appearance) has reduced strength and must be checked
1. Axial tension: σ=N/(lw·t) ≤ fwt
2. Axial compression: σ=N/(lw·t) ≤ fwc
3. Bending: σ=M/Ww ≤ fwt, Ww=t·lw²/6
4. Shear: τ=V·S/(I·t) ≤ fvv
5. Combined bending and shear: √(σ²+3τ²) ≤ 1.1·fwt
Grade 1: 100% inspection, dynamic/fatigue structures
Grade 2: 20% inspection, important structures
Grade 3: visual inspection, general structures
Plate thickness ≤6mm: I-groove
Plate thickness 6~20mm: V-groove
Plate thickness 20~50mm: X-groove
Plate thickness >30mm: U-groove (less filler)
τ = N/(he·lw) ≤ fwf
he — effective throat (=0.7·hf, hf is leg size)
lw — effective weld length (actual length minus 2hf)
fwf — design strength of fillet weld (MPa)
Q235+E43:fwf=160MPa
Q345+E50:fwf=200MPa
τ = N/(he·lw)·1.22 ≤ fwf
1.22 — strength increase factor for front weld
τ = N/(he·lw) ≤ fwf
σf = M/Wf ≤ 1.22·fwf
Wf = he·lw²/6
τf = V·Sf/If ≤ fwf
√((σf/1.22)² + τf²) ≤ fwf
Plate thickness t≤6mm: hf=t
Plate thickness 6 Plate thickness t>12: hf≥√t-1 (mm) hf ≤ 1.2t (t is thinner plate thickness) Fillet welding at edge: hf ≤ t-(1~2)mm T-joint, plate thickness 10mm, carrying N=200kN Leg hf=8mm, two side welds each 100mm long he=0.7×8=5.6mm lw=100-16=84mm (minus 2hf) τ=200000/(5.6×84×2)=213MPa > 200 → fails Increase leg size or add front weld[Maximum Leg Size hf_max]
[Minimum Effective Length] lw ≥ 8hf and ≥40mm
[Maximum Effective Length] lw ≤ 60hf (side weld; beyond this take 60hf but weld full length)
[Calculation Example]
Δσ ≤ [Δσ]
[Δσ] = (C/N)^(1/β)
Δσ — stress range (MPa) = σmax - σmin
[Δσ] — allowable stress range (MPa)
N — number of stress cycles
C, β — parameters (depend on weld detail category)
Category | C | Note
Z1 | 1920³ | unconnected base metal
Z2 | 1560³ | longitudinal butt weld
Z3 | 1120³ | transverse butt weld (grade 1)
Z4 | 692³ | cruciform joint
Z5 | 446³ | T-joint
Z6 | 405³ | side fillet weld
Z7 | 281³ | front fillet weld
Z8 | 204³ | weld end
Larger value means better fatigue performance
N ≤ C/[Δσ]^β
Σ(ni/Ni) ≤ 1
ni — number of cycles at each stress range level
Ni — fatigue life at that stress range
① Weld shape
Lower reinforcement is better (grinding flush raises 1~2 categories)
Concave fillet weld beats convex
② Defects
Cracks, lack of fusion, porosity severely degrade
Slag inclusions reduce by length
③ Residual stress
Large welding residual tensile stress should be relieved (annealing / vibratory aging)
① Keep welds away from high-stress zones
② Grind reinforcement flush on critical joints
③ Post-weld TIG remelting (toe remelting raises 2 categories)
④ Increase transition radius
⑤ Avoid dense/crossing welds
⑥ Use bolted joints instead of welds for fatigue-critical parts
Other quick references in this category:Mechanics fundamentalsFluid mechanicsVibrationThermodynamicsElectrical fundamentalsQuick calculation formulasHydraulic / inertia calculationGear strengthShaft strengthKey connectionSpringBolt strengthBeam and plate bending