E42-213 · Fatigue Fracture · Double-Speed Chain Conveyor · ★★★
After 1500h, link plate pin hole cracks; chain disengages and stops.
[Hole Edge Stress] Link plate pin hole without chamfer; edge stress concentration factor K_t=3.1; tensile σ=260MPa. [Fatigue Propagation] Under alternating tension, hole edge crack penetrates at 1500h. [Design Omission] Hole mouth not chamfered; plate thickness margin insufficient.
1. Chamfer both sides of pin hole mouth C1.
2. Increase link plate thickness from 6mm to 8mm.
3. Shot-peen hole edge for strengthening.
4. Raise chain pre-stretch load to 1.2x working load.
5. Harden pin surface to HRC55.
6. 100% inspection of chain length tolerance at shipment.
7. Shift-point inspection of link plate cracks.
8. Replace wearable chain links quarterly.
GB/T 1243-2006