E42-215 · Fatigue Fracture · Gantry Crane Main Girder · ★★★
After 2 years, crack at diaphragm cutout 120mm long, extending to web.
[Cutout Stress] Diaphragm has square hole for pipeline pass-through; hole edge sharp corner K_t=3.5; web stress σ=180MPa. [Fatigue Propagation] Under alternating hoist load, cutout crack grows 120mm in 2 years. [Design Omission] Cutout not rounded; not reinforced.
1. Change square hole corners to R10 radius.
2. Add reinforcement plate δ=10mm at hole edge.
3. Double-sided continuous weld diaphragm to web.
4. Calculate beam fatigue life ≥10⁶ cycles.
5. Set camber pre-deformation on main girder.
6. Shipment static load 1.25x test.
7. Annual magnetic-particle inspection by opening.
8. Grind weld toe to R2.
GB/T 3811-2008