Wrong Welding Sequence on an I-Beam Causes Angular Distortion Out of Tolerance

E42-010 · Weld Distortion & Defects · Gantry Welded Frame I-Beam · ★★★

Problem Symptom

After welding, web angular distortion 8mm/3m (allowable 3), correction cost is high

Root Cause

[Welding Heat Input] The single-pass heat input is E=UI/v=28×10/0.3=933kJ/m, and the transverse shrinkage is Δ≈0.2mm per pass × 12 passes.
[Angular Distortion] Welding one side first and then the other produces asymmetric shrinkage, giving an angular distortion θ=8mm/3000=0.0027rad, out of tolerance.
[Design Omission] No symmetric skip welding and no anti-deformation allowance were provided.

Correct Solution

1) Use symmetric segmented skip welding (300mm per segment);
2) Reserve 3mm of anti-deformation;
3) Reduce heat input (lower current / raise travel speed);
4) Clamp with welding jigs before welding to prevent displacement;
5) Flame-correct after welding and confirm ≤3mm;
6) Carry out vibration ageing after welding;
7) Inspect first-article deformation on a three-coordinate measuring machine;
8) Freeze the welding sequence on the process sheet and include it in first-article inspection.

Checklist

References

GB/T 19804-2005 Welding Structures — General Requirements